Minimum Bend Radius Chart

Minimum bend radius recommendations for sheet metal by material type, thickness, and grain direction. Covers aluminum (5052-H32, 6061-T6), mild steel, 304 stainless steel, C110 copper, and C260 brass across common gauges.

Minimum Bend Radius Chart

MATERIALALLOY / GRADETHICKNESS (IN)GAUGEMIN RADIUS (WITH GRAIN)MIN RADIUS (ACROSS GRAIN)NOTES
Aluminum5052-H320.02024 ga1T (0.020″)0.5T (0.010″)Most formable common alloy
Aluminum5052-H320.03222 ga1T (0.032″)0.5T (0.016″)Excellent for enclosures
Aluminum5052-H320.04020 ga1T (0.040″)1T (0.040″)General sheet metal work
Aluminum5052-H320.06316 ga1T (0.063″)1T (0.063″)Brackets, panels
Aluminum5052-H320.09013 ga1.5T (0.135″)1T (0.090″)Structural panels
Aluminum5052-H320.12511 ga1.5T (0.188″)1T (0.125″)Heavier brackets
Aluminum6061-T60.03222 ga3T (0.096″)2T (0.064″)Prone to cracking; anneal for tighter bends
Aluminum6061-T60.04020 ga3T (0.120″)2T (0.080″)Use generous radii
Aluminum6061-T60.06316 ga4T (0.252″)3T (0.189″)Consider 5052 if tight bends needed
Aluminum6061-T60.09013 ga5T (0.450″)3T (0.270″)High risk of cracking
Aluminum6061-T60.12511 ga6T (0.750″)4T (0.500″)Anneal bend zone recommended
Aluminum6061-T60.19010 ga6T (1.140″)5T (0.950″)Not recommended for tight bends
Mild Steel1018 CR0.03022 ga0.5T (0.015″)0.5T (0.015″)Very formable
Mild Steel1018 CR0.04818 ga0.5T (0.024″)0.5T (0.024″)General fabrication
Mild Steel1018 CR0.06016 ga1T (0.060″)0.5T (0.030″)Brackets, chassis
Mild Steel1018 CR0.07514 ga1T (0.075″)0.5T (0.038″)Structural parts
Mild Steel1018 CR0.10512 ga1T (0.105″)1T (0.105″)Heavy gauge forming
Mild Steel1018 CR0.13510 ga1.5T (0.203″)1T (0.135″)Heavy gauge, may need bottoming
Stainless Steel304 (annealed)0.03022 ga1T (0.030″)0.5T (0.015″)Work hardens during bending
Stainless Steel304 (annealed)0.04818 ga1T (0.048″)0.5T (0.024″)General stainless fabrication
Stainless Steel304 (annealed)0.06016 ga1T (0.060″)1T (0.060″)Kitchen, medical equipment
Stainless Steel304 (annealed)0.07514 ga1.5T (0.113″)1T (0.075″)Heavier stainless parts
Stainless Steel304 (annealed)0.10512 ga1.5T (0.158″)1T (0.105″)Structural stainless
Stainless Steel304 (annealed)0.13510 ga2T (0.270″)1.5T (0.203″)High springback; over-bend required
CopperC110 (ETP, soft)0.02024 ga0T (flat)0T (flat)Extremely ductile when annealed
CopperC110 (ETP, soft)0.03222 ga0T (flat)0T (flat)Bus bars, electrical
CopperC110 (ETP, soft)0.06316 ga0.5T (0.032″)0T (flat)Excellent formability
CopperC110 (ETP, soft)0.12511 ga1T (0.125″)0.5T (0.063″)Heavier bus bars
BrassC260 (cartridge, soft)0.02024 ga0T (flat)0T (flat)Very ductile annealed brass
BrassC260 (cartridge, soft)0.03222 ga0.5T (0.016″)0T (flat)Decorative, musical instruments
BrassC260 (cartridge, soft)0.06316 ga0.5T (0.032″)0.5T (0.032″)General brass fabrication
BrassC260 (cartridge, soft)0.12511 ga1T (0.125″)0.5T (0.063″)Heavier brass parts
BrassC260 (half-hard)0.03222 ga1T (0.032″)0.5T (0.016″)Springs, clips
BrassC260 (half-hard)0.06316 ga1.5T (0.095″)1T (0.063″)Structural brass
CopperC110 (half-hard)0.06316 ga1T (0.063″)0.5T (0.032″)Harder temper; less ductile
CopperC110 (half-hard)0.12511 ga2T (0.250″)1T (0.125″)Anneal for tighter bends

Quick Answer: What Is the Minimum Bend Radius for Sheet Metal?

The minimum bend radius is the smallest inside radius you can bend a sheet to without cracking the outer surface. It is set by the material, temper, thickness and grain direction. It is stated as a multiple of thickness (T). Soft tempers like annealed copper or 5052-H32 aluminum bend to about 0.5T–1T, while hard 6061-T6 aluminum needs 3T–6T to avoid fracture.

This chart lists minimum inside bend radius by material, alloy and gauge for 90° bends, with separate values for bending with the grain (worst case) and across the grain (best case), plus practical notes. Inputs are the material/alloy, the sheet thickness or gauge and the grain orientation relative to the bend line.

Common minimums: 5052-H32 aluminum → 1T | 6061-T6 aluminum → 3T–6T | 1018 mild steel → 0.5T–1T | 304 stainless → 1T–2T | annealed C110 copper & C260 brass → 0T–1T | bend across the grain for tighter radii.

Notes on This Chart

  • “T” refers to material thickness. Example: 2T for 0.063″ material = 0.126″ minimum bend radius.
  • Values are for 90-degree bends. Sharper angles may require larger radii.
  • “With grain” means bending parallel to the rolling direction (worst case). “Across grain” is perpendicular (best case).
  • Actual results vary with tooling condition, press brake tonnage, and material lot variation.
  • When in doubt, test bend a sample piece before committing to production.
  • Bending with the grain direction reduces formability; always design bends perpendicular (across) the material grain to prevent stress fractures.

Need Precision Sheet Metal Bending and Fabrication?

We offer quick-turn sheet metal laser cutting, bending, and insert services with standard bend radii. Upload your CAD drawings for an instant quote.

Frequently Asked Questions

What is the minimum bend radius for sheet metal?

The minimum bend radius is the smallest inside radius that can be used without causing cracking or permanent damage to the sheet. It varies by material, thickness, temper, and grain direction. Ductile materials such as soft aluminum can typically use tighter radii, while harder materials such as 6061-T6 aluminum require larger bend radii.

Grain direction affects how sheet metal responds to bending. Bending across the grain generally allows tighter radii and reduces the risk of cracking, while bending along the grain requires a larger radius. For critical bends, consider the rolling direction when designing the part and orient bends across the grain whenever possible.

Using a bend radius smaller than recommended can cause cracking, splitting, or surface deformation on the outside of the bend. Harder materials and tempers are especially susceptible to cracking. Following the recommended minimum radius helps maintain part integrity and reduces the risk of forming defects.

Bend allowance can be calculated using the bend angle, inside bend radius, material thickness, and K-factor:

Bend Allowance = (π / 180) × Bend Angle × (Bend Radius + K-factor × Material Thickness)

The appropriate K-factor depends on the forming method and material. Use the actual values from your press brake setup or material specifications for accurate flat-pattern calculations.

Yes, but 6061-T6 aluminum requires larger bend radii than more formable alloys such as 5052-H32. Depending on material thickness, a radius of approximately 3T to 6T may be required. Bending across the grain and using a larger radius can reduce cracking. For tighter bends, consider using 5052-H32 or annealing the 6061 material before forming.