Minimum Bend Radius Chart
Minimum bend radius recommendations for sheet metal by material type, thickness, and grain direction. Covers aluminum (5052-H32, 6061-T6), mild steel, 304 stainless steel, C110 copper, and C260 brass across common gauges.
Minimum Bend Radius Chart
| MATERIAL | ALLOY / GRADE | THICKNESS (IN) | GAUGE | MIN RADIUS (WITH GRAIN) | MIN RADIUS (ACROSS GRAIN) | NOTES |
| Aluminum | 5052-H32 | 0.020 | 24 ga | 1T (0.020″) | 0.5T (0.010″) | Most formable common alloy |
| Aluminum | 5052-H32 | 0.032 | 22 ga | 1T (0.032″) | 0.5T (0.016″) | Excellent for enclosures |
| Aluminum | 5052-H32 | 0.040 | 20 ga | 1T (0.040″) | 1T (0.040″) | General sheet metal work |
| Aluminum | 5052-H32 | 0.063 | 16 ga | 1T (0.063″) | 1T (0.063″) | Brackets, panels |
| Aluminum | 5052-H32 | 0.090 | 13 ga | 1.5T (0.135″) | 1T (0.090″) | Structural panels |
| Aluminum | 5052-H32 | 0.125 | 11 ga | 1.5T (0.188″) | 1T (0.125″) | Heavier brackets |
| Aluminum | 6061-T6 | 0.032 | 22 ga | 3T (0.096″) | 2T (0.064″) | Prone to cracking; anneal for tighter bends |
| Aluminum | 6061-T6 | 0.040 | 20 ga | 3T (0.120″) | 2T (0.080″) | Use generous radii |
| Aluminum | 6061-T6 | 0.063 | 16 ga | 4T (0.252″) | 3T (0.189″) | Consider 5052 if tight bends needed |
| Aluminum | 6061-T6 | 0.090 | 13 ga | 5T (0.450″) | 3T (0.270″) | High risk of cracking |
| Aluminum | 6061-T6 | 0.125 | 11 ga | 6T (0.750″) | 4T (0.500″) | Anneal bend zone recommended |
| Aluminum | 6061-T6 | 0.190 | 10 ga | 6T (1.140″) | 5T (0.950″) | Not recommended for tight bends |
| Mild Steel | 1018 CR | 0.030 | 22 ga | 0.5T (0.015″) | 0.5T (0.015″) | Very formable |
| Mild Steel | 1018 CR | 0.048 | 18 ga | 0.5T (0.024″) | 0.5T (0.024″) | General fabrication |
| Mild Steel | 1018 CR | 0.060 | 16 ga | 1T (0.060″) | 0.5T (0.030″) | Brackets, chassis |
| Mild Steel | 1018 CR | 0.075 | 14 ga | 1T (0.075″) | 0.5T (0.038″) | Structural parts |
| Mild Steel | 1018 CR | 0.105 | 12 ga | 1T (0.105″) | 1T (0.105″) | Heavy gauge forming |
| Mild Steel | 1018 CR | 0.135 | 10 ga | 1.5T (0.203″) | 1T (0.135″) | Heavy gauge, may need bottoming |
| Stainless Steel | 304 (annealed) | 0.030 | 22 ga | 1T (0.030″) | 0.5T (0.015″) | Work hardens during bending |
| Stainless Steel | 304 (annealed) | 0.048 | 18 ga | 1T (0.048″) | 0.5T (0.024″) | General stainless fabrication |
| Stainless Steel | 304 (annealed) | 0.060 | 16 ga | 1T (0.060″) | 1T (0.060″) | Kitchen, medical equipment |
| Stainless Steel | 304 (annealed) | 0.075 | 14 ga | 1.5T (0.113″) | 1T (0.075″) | Heavier stainless parts |
| Stainless Steel | 304 (annealed) | 0.105 | 12 ga | 1.5T (0.158″) | 1T (0.105″) | Structural stainless |
| Stainless Steel | 304 (annealed) | 0.135 | 10 ga | 2T (0.270″) | 1.5T (0.203″) | High springback; over-bend required |
| Copper | C110 (ETP, soft) | 0.020 | 24 ga | 0T (flat) | 0T (flat) | Extremely ductile when annealed |
| Copper | C110 (ETP, soft) | 0.032 | 22 ga | 0T (flat) | 0T (flat) | Bus bars, electrical |
| Copper | C110 (ETP, soft) | 0.063 | 16 ga | 0.5T (0.032″) | 0T (flat) | Excellent formability |
| Copper | C110 (ETP, soft) | 0.125 | 11 ga | 1T (0.125″) | 0.5T (0.063″) | Heavier bus bars |
| Brass | C260 (cartridge, soft) | 0.020 | 24 ga | 0T (flat) | 0T (flat) | Very ductile annealed brass |
| Brass | C260 (cartridge, soft) | 0.032 | 22 ga | 0.5T (0.016″) | 0T (flat) | Decorative, musical instruments |
| Brass | C260 (cartridge, soft) | 0.063 | 16 ga | 0.5T (0.032″) | 0.5T (0.032″) | General brass fabrication |
| Brass | C260 (cartridge, soft) | 0.125 | 11 ga | 1T (0.125″) | 0.5T (0.063″) | Heavier brass parts |
| Brass | C260 (half-hard) | 0.032 | 22 ga | 1T (0.032″) | 0.5T (0.016″) | Springs, clips |
| Brass | C260 (half-hard) | 0.063 | 16 ga | 1.5T (0.095″) | 1T (0.063″) | Structural brass |
| Copper | C110 (half-hard) | 0.063 | 16 ga | 1T (0.063″) | 0.5T (0.032″) | Harder temper; less ductile |
| Copper | C110 (half-hard) | 0.125 | 11 ga | 2T (0.250″) | 1T (0.125″) | Anneal for tighter bends |
Quick Answer: What Is the Minimum Bend Radius for Sheet Metal?
The minimum bend radius is the smallest inside radius you can bend a sheet to without cracking the outer surface. It is set by the material, temper, thickness and grain direction. It is stated as a multiple of thickness (T). Soft tempers like annealed copper or 5052-H32 aluminum bend to about 0.5T–1T, while hard 6061-T6 aluminum needs 3T–6T to avoid fracture.
This chart lists minimum inside bend radius by material, alloy and gauge for 90° bends, with separate values for bending with the grain (worst case) and across the grain (best case), plus practical notes. Inputs are the material/alloy, the sheet thickness or gauge and the grain orientation relative to the bend line.
Common minimums: 5052-H32 aluminum → 1T | 6061-T6 aluminum → 3T–6T | 1018 mild steel → 0.5T–1T | 304 stainless → 1T–2T | annealed C110 copper & C260 brass → 0T–1T | bend across the grain for tighter radii.
Notes on This Chart
- “T” refers to material thickness. Example: 2T for 0.063″ material = 0.126″ minimum bend radius.
- Values are for 90-degree bends. Sharper angles may require larger radii.
- “With grain” means bending parallel to the rolling direction (worst case). “Across grain” is perpendicular (best case).
- Actual results vary with tooling condition, press brake tonnage, and material lot variation.
- When in doubt, test bend a sample piece before committing to production.
- Bending with the grain direction reduces formability; always design bends perpendicular (across) the material grain to prevent stress fractures.
Need Precision Sheet Metal Bending and Fabrication?
We offer quick-turn sheet metal laser cutting, bending, and insert services with standard bend radii. Upload your CAD drawings for an instant quote.
Frequently Asked Questions
What is the minimum bend radius for sheet metal?
The minimum bend radius is the smallest inside radius that can be used without causing cracking or permanent damage to the sheet. It varies by material, thickness, temper, and grain direction. Ductile materials such as soft aluminum can typically use tighter radii, while harder materials such as 6061-T6 aluminum require larger bend radii.
Why does grain direction matter when bending sheet metal?
Grain direction affects how sheet metal responds to bending. Bending across the grain generally allows tighter radii and reduces the risk of cracking, while bending along the grain requires a larger radius. For critical bends, consider the rolling direction when designing the part and orient bends across the grain whenever possible.
What happens if I bend sheet metal below the minimum radius?
Using a bend radius smaller than recommended can cause cracking, splitting, or surface deformation on the outside of the bend. Harder materials and tempers are especially susceptible to cracking. Following the recommended minimum radius helps maintain part integrity and reduces the risk of forming defects.
How do I calculate bend allowance for sheet metal?
Bend allowance can be calculated using the bend angle, inside bend radius, material thickness, and K-factor:
Bend Allowance = (π / 180) × Bend Angle × (Bend Radius + K-factor × Material Thickness)
The appropriate K-factor depends on the forming method and material. Use the actual values from your press brake setup or material specifications for accurate flat-pattern calculations.
Can I bend 6061-T6 aluminum without cracking?
Yes, but 6061-T6 aluminum requires larger bend radii than more formable alloys such as 5052-H32. Depending on material thickness, a radius of approximately 3T to 6T may be required. Bending across the grain and using a larger radius can reduce cracking. For tighter bends, consider using 5052-H32 or annealing the 6061 material before forming.